Investigation of Both Electrolyte Supply Method and Membrane Thickness for Anion Exchange Membrane Water Electrolysis Cells Under High Current-Density Operation
Anion exchange membrane water electrolysis (AEMWE) has the same membrane electrode assembly (MEA) structure as proton exchange membrane water electrolysis (PEMWE), and because the system is alkaline, non-precious metals can be used. Therefore, AEMWEs have the potential to be as low in cost as alkaline water electrolysis (AWE) and as high in current density as PEMWEs. 1 Practical application is also expected, and it is becoming necessary to investigate comprehensively operating conditions such as the electrolyte supply method and current density. In this study, we fabricated an MEA using a non-precious metal catalyst, Ni0.80Fe0.20OX 2, developed at the University of Yamanashi (UY) as the anode and a partially fluorinated hydrocarbon-based anion-exchange electrolyte QPAF-43 developed at UY as the electrolyte membrane and binder, and evaluated the cell as well as the electrolyte supply method.The catalyst ink for the anode was prepared by mixing the Ni0.80Fe0.20Ox catalyst (UY) with solvent (water/methanol) and QPAF-4 (IEC = 1.5 meq g-1, UY) binder solution. The anode ink was coated by use of pulse-swirl-spray (PSS, Nordson) on the QPAF-4 membranes (thickness 50 or 30 μm, IEC = 1.5 meq g-1) to make the catalyst-coated membranes (CCMs) with the anode. The catalyst ink for the cathode was prepared by mixing Pt/CB catalyst (TEC10E50E, TANAKA) with solvent (water/methanol) and QPAF-4 (IEC = 2.0 meq g-1) binder solution. The cathode ink was coated by using PSS on the opposite side of the CCM. Ni mesh (Bekaert) and carbon paper (TGP-H-120, Toray) were used for the anode and cathode porous transport layers (PTLs), respectively. The single cell (Figure 1, cell structure developed at Yokohama National University) performances were measured while supplying 1 M KOH at 80 °C.Figures 2a and 2b show the polarization curves and cell resistance (at 10 kHz) up to a current density of 10 A cm-2 for electrolyte supplied to both electrodes (both-side supply, membrane thickness 50 μm) and electrolyte supplied to the anode side only (anode-side supply, membrane thickness 50 μm or 30 μm). For the both-side supply, 50 μm membrane thickness, there was no significant increase in cell voltage and resistance, but for the anode-side supply, 50 μm membrane thickness, there was a significant increase in cell voltage and resistance in the current density range of 3 A cm-2 or more. On the other hand, with the anode-side supply, 30 μm membrane thickness, there was no significant increase in cell voltage and resistance. This is thought to be a result of the improved water supply from the anode to the cathode via the membrane due to the thinner membrane.From these results, it is suggested that both increasing the amount of water permeating through the membrane and designing a cathode catalyst layer that is suitable for water holding are important when the electrolyte is supplied to the anode side only. Acknowledgement This work was partially based on results obtained from project JPNP20003, commissioned by the New Energy and Industrial Technology Development Organization (NEDO). References N. Du, C. Roy, R. Peach, M. Turnbull, S. Thiele, and C. Bock, Chem. Rev. 122, 11830 (2022).G. Shi, C. Arata, D. A. Tryk, T. Tano, M. Yamaguchi, A. Iiyama, M. Uchida, K. Iida, S. Watanabe, and K. Kakinuma, ACS Omega 8, 13068 (2023).H. Ono, T. Kimura, A. Takano, K. Asakawa, J. Miyake, J. Inukai, and K. Miyatake, J. Mater. Chem. A 5, 24804 (2017). Figure 1
Read more